Quick answer: If your LSZH compound passes the burn test but arrives with poor elongation, gels or an inconsistent melt index between lots, the formulation is probably fine and the process is not. At 60 % mineral loading the LSZH cable compound production process has almost no tolerance left — feed order, melt temperature and screw configuration decide the mechanical result more than the recipe does.
Buyers ask us for a formulation. Compounders who have actually run this material ask a different question: how is it fed, and at what temperature. That second question is the one that separates a compound you can extrude at line speed from one that looks right on paper.
Why this material is hard to make
An LSZH cable compound is not a polymer with additives in it. At 55–65 % aluminium trihydroxide or magnesium hydroxide flame retardant by weight, it is a mineral held together by just enough polymer to extrude. Every processing decision follows from that one fact.
Two constraints run against each other the whole way through. You need enough shear to wet out and disperse the filler, because undispersed mineral is both a mechanical defect and a flame-performance defect. But the filler decomposes endothermically — that is the entire flame retardant mechanism — and ATH starts releasing its water around 200 °C. Shear generates heat. So you are trying to disperse hard while staying cool, using a material whose whole purpose is to react to heat.
That is why heavily filled halogen-free work sits on co-rotating twin-screws rather than single screws, and why the practical advice is controlled shear rather than brute force: the screw has to disperse without cooking the filler.
Choose a Feed Arrangement for the Formulation and Line
Mineral loading, powder handling and available screw configuration can make feeding an important part of LSZH compounding. There is no single throat-and-side-feeder sequence that should be treated as mandatory for every formulation or machine. Obtain the compound development recommendations and confirm the proposed arrangement with the equipment and material suppliers.
One arrangement to investigate is melting the polymer before adding part of the mineral through a suitable downstream feeder. Other systems may require a different sequence. Use the following as a trial-planning checklist, not a prescribed recipe.
| Line element | Question to investigate | Record during the trial |
|---|---|---|
| Main feed | Can the system meter and convey the proposed feed consistently? | Feed rates and output stability |
| Downstream mineral addition | Is the port, feeder and screw arrangement suitable? | Pressure, torque and evidence of unstable feeding |
| Mixing | Does the selected setup produce the required dispersion? | Melt conditions, dispersion and mechanical results |
| Venting and material handling | Are moisture and volatile-control requirements met? | Handling conditions, vent performance and visible defects |
Specify the screw design, available feeding and venting equipment, throughput target and wear requirements with the equipment supplier. A fixed L/D ratio or barrel material is not a universal qualification for LSZH production. Evaluate whether the actual setup can maintain the required process conditions and finished compound properties.
Evaluate Filler Treatment and Coupling Together
Compare the proposed filler treatment with the polymer blend, coupling chemistry and processing route. Pre-treated filler and treatment during compounding are options to discuss with the suppliers; neither description guarantees the required properties.
Huber’s surface-treated ATH literature explains the role of filler-polymer compatibility and provides grade-specific examples. Nabaltec’s cable formulation examples evaluate filler characteristics and coupling systems together. These are manufacturer examples, not performance guarantees for another formulation.
Agree the material handling and moisture requirements with the suppliers. Compare matched trials for tensile strength, elongation, dispersion and the other specified properties. Keep the final result tied to the tested formulation and processing conditions rather than assigning one elongation value to a coating or coupling-agent label.
Where crosslinked grades change the picture
For grades that need heat resistance beyond thermoplastic HFFR, silane crosslinking is the usual route: a vinyl silane such as VTMS or VTES is grafted onto the polymer during compounding in the presence of an organic peroxide, and the crosslinks form later when the extruded cable is exposed to moisture with a catalyst present.
The practical consequence is that a silane-crosslinkable LSZH compound has a shelf life and a moisture-sensitive storage requirement that a plain thermoplastic grade does not. We have had material land in a humid port warehouse for six weeks and start reacting in the bag. If your grade is crosslinkable, ask about storage before you ask about price.
Investigate Surface Defects Without Assuming the Cause
As a hypothetical troubleshooting example, a cable producer may observe intermittent roughness even though its tested specimens meet the specified fire requirements. This is an investigation scenario, not a documented Rectivas customer lot. An acceptable fire result does not answer a separate appearance or dimensional requirement.
Record when the defect appears and compare it with feeder output, torque, melt pressure, material identity, tooling condition and the processing history. Review the retained material and the line conditions before changing the chemistry. A controlled change to the feed arrangement can test a feeding hypothesis, but improvement alone does not establish a universal fault or a guaranteed remedy.
Retain the trial settings and repeat the relevant appearance, mechanical and fire checks before approving a production change. For the separate scope of smoke evidence, see the smoke density test guide. No trial volume, diagnostic timeline or customer result is claimed here.
What you can check without visiting the plant
Most buyers cannot audit a compounding line, and honestly most audits that do happen look at paperwork rather than screw configuration. Three things you can ask for that actually tell you something:
Melt index or melt volume rate across lots, not just within one. Lot-to-lot MFI drift on a heavily filled compound usually means thermal history is varying, which means the process is not under control.
Elongation at break on the compound, not the cable. If the compound leaves at 150 % and the cable tests at 120 %, that is your extrusion. If the compound itself is at 100 %, it was made that way.
Ash content or filler content per lot. Cheap to run, and it catches the substitution that a burn test will not: a compound quietly re-balanced toward more filler and less polymer still passes the flame test and loses mechanicals.
Ask for a grade-specific window using the flame retardant processing temperature guide; decomposition data alone do not define safe production settings.
What we would actually advise
If you compound in-house: fix the feed configuration before touching the recipe. Split the filler across two side feeders, keep the melt under the ATH decomposition onset, and use pre-coated filler while you are still stabilising the process — move to in-situ treatment later if the volume justifies it. The general processability rules across all flame retardant families are in compounding flame retardants.
If you extrude cable but do not compound: do not start now. At 60 % loading the capital and the learning curve are real, and a finished flame retardant compound is almost always the cheaper answer for a cable maker. This is one of the few cases where we will actively talk you out of the additive route.
If the cable goes outdoors: the filler coating decision is no longer only about dispersion — it also decides weathering life, which is set out in UV resistant LSZH compound.
If you are qualifying a new supplier: ask for three consecutive lot COAs rather than one. A single good lot proves a good day. Three consecutive lots start to prove a process.
Before comparing delivered tonnes or cable yield, check how LSZH compound density affects cable length per tonne using the actual jacket geometry.
If the jacket retracts after extrusion or conditioning, follow the LSZH jacket shrinkback investigation to compare the test and process history before replacing the grade.
FAQ
What is the LSZH cable compound production process, in short?
Polymer and coupling agent at the main throat, a melt seal established, then 55–65 % ATH or MDH fed downstream through one or two side feeders into the existing melt, distributive mixing at controlled shear, vacuum devolatilisation, then pelletising. The order matters more than the ingredient list.
Why can’t the filler go in at the main feed throat?
Bulk density and air entrainment. Mineral powder at that proportion starves the feed section and causes surging, which the operator usually corrects with screw speed, which adds heat where you least want it. Side feeding puts the filler into a melt that can wet it immediately.
What melt temperature limit applies?
ATH begins releasing water around 200 °C, so the melt has to stay below that with margin. MDH decomposes around 330 °C and gives a much wider window, which is the main technical reason to pay more for it. Choosing between them is covered on our halogen-free flame retardant page.
Should I buy pre-coated filler or treat it in-situ?
Pre-coated while you are stabilising, in-situ once your process is repeatable and the volume justifies the saving. In-situ treatment makes your dispersion depend on residence time and moisture control on the day, which is a poor trade when you are still learning the material.
Can I make LSZH compound on a single screw?
Not well at these loadings. Heavily filled halogen-free work belongs on a co-rotating twin-screw with side feeding and vacuum venting. A single screw cannot feed the filler downstream or devolatilise properly.
Why does my compound pass the burn test but fail mechanically?
Because flame performance is driven by how much filler is present and mechanical performance by how well it is bonded and dispersed. You can have the first without the second. Check elongation and filler content per lot, not just the flame result.
Do you supply the compound or only the additives?
Both. Flame retardant additives as powder packages for compounders and finished compound for cable makers who do not compound. We are a sourcing and technical partner rather than a factory owner, so the compound is produced at the partner factory whose line suits the grade, with UL94 and LOI screening we arrange and cable-level reports through an accredited laboratory. Cable standards and the wider system view sit on the flame retardant for wire and cable page.
Final thoughts
The recipe for an LSZH compound is not a secret and has not been for twenty years. What separates lots that run from lots that do not is process discipline at a filler loading that leaves no margin: where the mineral enters, how hot it gets, whether the coupling agent had dry surfaces to react with. When a compound underperforms, look at the process trace before the formulation sheet — in our experience that is where the answer is more often than not. Send the standard you have to meet, your line speed and your elongation minimum, and we will tell you which route fits, including when the honest answer is to buy finished compound instead of learning to make it. The filler grade you feed matters as much as how you feed it; surface area and purity are covered in flame retardant filler selection.
—— Rectivas Materials 团队 技术工程师老陈